+86-159-2181-9772 | ben.liu@ulilaser.com

Laser Solder Paste vs Solder Ring on an EPS Motor Controller: A Real Trial

Application note · Automotive

Laser Solder Paste vs Solder Ring on an EPS Motor Controller: A Real Trial

Test date: 26 March 2026 · Process: laser solder paste (with a solder ring run for comparison) · Part: EPS steering motor controller · 500 W / 915 nm

EPS steering motor controller pads before and after laser solder paste soldering
Featured image, composed from this test’s own photos: the controller before soldering (left) and the paste-soldered result (right).

Steering is the one system in a car where a marginal joint is not a warranty issue, it is a safety issue. That is why EPS motor controllers get large power pads, heavy copper and through-holes that hold a lot of solder — and why those pads are surprisingly hard to solder with a concentrated heat source.

In March we ran a comparative trial on exactly this part for a Tier-1 steering system supplier in Jiangsu. The board carries four oval power pads, each close to 8 mm across, with through-holes open in the middle. Two process routes were tested on the same pads: a solder ring placed on the pad, and solder paste pre-deposited on the pad. One route failed and one route passed. The reason the ring failed is the part worth reading, because it has nothing to do with laser power.

The part, and why it is difficult

The workpiece is the motor controller PCBA from an electric power steering unit. Four oval pads carry the phase terminals. Each pad has a through-hole, so the joint is not a flat surface — it is a pad with a hole in the middle that solder is expected to fill.

Three properties of this geometry drive the whole process:

  • Large thermal mass. An 8 mm pad on heavy copper pulls heat away from the joint far faster than a fine-pitch pad. Whatever energy the laser delivers has to be enough to heat the pad, not just the point under the beam.
  • A hole in the measurement zone. The hole is inside the heated area. Any temperature sensor aimed at the pad centre sees the hole as the pad melts and opens up — and a hole is not at solder temperature.
  • Solder mask close to the pad edge. The gap between pad and mask is small, and 915 nm light reflects off a shiny molten surface. Anything that reflects lands on the mask around the pad.
EPS motor controller power pads with pre-deposited solder paste and laser alignment spot
The sample before soldering: oval power pads with through-holes, paste pre-deposited, and the red laser alignment spot visible on the pad.

Trial setup

Both routes used the same optical configuration. Values below are exactly as recorded in the test report.

Laser module power 500 W
Wavelength 915 nm
Fiber core diameter 200 µm
Focal length / working distance 100 mm / 100 mm
Spot diameter 8 mm, circular
Solder alloy SAC305, 13 % flux
Paste deposition Manual, pre-deposited on pad
Workpiece angle / head angle 0° / 90°
Ambient conditions 20 °C, 45 % RH

Route A — the solder ring, and why it failed

A solder ring was placed on the pad and heated until it flowed. Mechanically this is the tidier option: the solder volume is fixed by the ring, no dispensing step is needed, and the ring sits where the joint needs metal.

It failed on temperature control, not on solder volume. As the ring melted, the through-hole became visible again. The infrared sensor was measuring the pad area that now contained an open hole, so the reading no longer represented the pad surface. The controller saw a lower temperature than the pad actually needed to reach, cut the energy short, and the pad never got enough heat. The report records the run as NG — insufficient heat on the pad, with the ring already consumed.

Why this matters beyond one part: any pad with an open hole has this problem. The moment the filler metal uncovers the hole, a single-point IR reading becomes unreliable. Adding power does not fix it — it only makes the error larger. The fix is either a measurement point off the hole, or a process where the hole stays covered.

This is the same class of problem we describe in closed-loop temperature control for laser solder paste: a control loop is only as good as the point it measures.

Route B — solder paste, and what worked

The second route pre-deposited SAC305 paste on each pad. Because paste covers the hole before heating starts, the measured spot stays on solder for the whole cycle. The heating program was stepped rather than a single pulse:

Step 1 150 → 280 °C, ramp 1500 ms
Dwell at 280 °C 2000 ms
Step 2 280 → 380 °C, ramp 1500 ms
Dwell at 380 °C 4500 ms
Peak temperature 380 °C
Single-point heating time 6500 ms
Laser soldering software command editor showing stepped temperature and time instructions
The stepped program used in the trial, captured from the machine’s command editor: two temperature ramps with holds, not a single pulse.

The report records the pads as solderable: the paste filled and wetted the joints on all four positions. Two defects remained, and the report names both rather than hiding them.

  • Spatter and residue. Small solder beads and flux residue sat on the mask around the pads after soldering. This is normal for paste without a cleaning step, but it is not acceptable on a safety-relevant board.
  • Solder mask scorching. The 8 mm circular spot matched the pad length, so its edge fell on the mask. Reflected light from the molten surface burned the mask at the pad boundary.
EPS controller pads after laser solder paste soldering, showing solder beads and flux residue around the joints
After the paste run: joints are formed and wetting is complete, but solder beads and flux residue remain on the surrounding mask.

We are not going to quote a yield figure here, because the report does not contain one. It records solderability as OK on this sample and lists the two defects above. Any article claiming a percentage from this test would be making it up.

What we would change before production

  1. Switch from a round to a bar-shaped optic. The pad is oval; an 8 mm circle overshoots it at the sides. A bar spot slightly shorter than the pad keeps the beam inside the copper and stops the mask from being the thing that absorbs the reflection. This was the report’s own first recommendation.
  2. Add a cleaning station. Paste on a 915 nm process leaves residue. If the board cannot be washed, the paste volume and flux type have to be re-selected before this route is production-ready.
  3. Replace the temporary fixture. The sample was held with a temporary measure during the trial. Pad position repeatability is what makes an 8 mm spot land in the same place every cycle.
  4. Measure off the hole, not through it. If a ring or any hole-filling route is revisited, the temperature sensor must be aimed at a solid part of the pad that stays covered for the whole cycle.

Where low-temperature alloys fit on EV power modules

This trial ran SAC305 with a 380 °C peak, and for a bare FR4 power pad that is a workable number. It stops being workable when the same joint sits next to connectors, plastics or sensors that cannot see 380 °C. That is the case where a low-temperature alloy earns its place on EV power modules: the peak drops, the thermal load on everything around the pad drops with it, and the process window widens enough to protect the assembly rather than just the joint.

The trade-off is mechanical. Lower melting point usually means lower joint strength and a narrower margin against service temperature, so the alloy has to be chosen against the module’s real thermal environment, not picked because it is easier to solder. On this controller the paste route passed at 380 °C, so there was no reason to move down; on a module with tighter thermal neighbours, the calculation changes.

A checklist for your own EPS pad trial

  • Check whether the pad has an open through-hole before choosing a solder ring. If it does, plan the temperature measurement around it.
  • Match spot geometry to pad geometry — oval pad, bar spot. A circle will always spill onto the mask at the short sides.
  • Step the heating profile. Two ramps with holds gave a stable joint here; a single pulse gives the controller no chance to correct.
  • Budget a cleaning step for any paste route, and inspect for beads before the board moves on.
  • Fix the part repeatably before tuning power and time.
  • Inspect the joint with AOI if the volume justifies it — the bead and residue defects in this trial are exactly what inline AOI for laser solder joints is built to catch.

FAQ

Why did the solder ring fail while the paste worked on the same pad?

Because of what the temperature sensor could see. As the ring melted, the through-hole opened up, so the infrared reading stopped representing the pad surface. The controller under-heated the pad. Paste covers the hole from the start, so the measurement stayed valid through the whole cycle.

Can I just increase laser power to make the ring route work?

No. If the sensor is reading the hole instead of the pad, more power does not correct the reading, it only increases the error. The measurement point has to be moved off the hole, or the hole has to stay covered during heating.

Is an 8 mm circular spot right for these pads?

It worked, but it is not the right shape. The pads are oval, so a circular spot reaches the solder mask at the short sides and causes the scorching recorded in this trial. A bar-shaped spot slightly shorter than the pad is the better match.

Should I use low-temperature paste on an EV power module?

Use it when the parts around the joint cannot survive a high peak. Lower peak temperature protects connectors, plastics and sensors, but it also reduces joint strength and the margin against service temperature. Decide with the module’s thermal environment in hand, not by default.

Why is there solder spatter around the joints?

Paste processes produce beads and flux residue, and this trial recorded both. The report’s recommendation is a cleaning station; the alternative is to re-select paste volume and flux type so less residue is generated in the first place.

The one-line takeaway: on a pad with a through-hole, the process that keeps the hole covered is the process that keeps the temperature reading honest. That, not laser power, is what separated the two routes here.

Soldering power pads with through-holes?

Send us the pad drawing and the board stack-up. We will run both routes on our laser soldering platform and return a parameter sheet with before-and-after photos, the way this note was built. Consumables are covered under lead-free solder paste.

Source: internal test report 20260326A, 26 March 2026 — laser solder paste, 500 W / 915 nm, 8 mm circular spot, SAC305 with 13 % flux, 380 °C peak, 6500 ms single-point time, 20 °C / 45 % RH. All parameters, photographs and conclusions in this article are taken from that single test record.

Need Help?

Tell us about your application — our engineers will recommend the right solution.

Talk to an Engineer