Laser Solder Wire vs Solder Paste on a Radar Module: Same Pins, Two Processes

Application note · Automotive radar

Laser Solder Wire vs Solder Paste on a Radar Module: Same Pins, Two Processes

Test date: 26 March 2026 · Part: radar sensor module, 2 × 3 through-hole pins in oval ring pads · 200 W / 915 nm

Laser soldered radar module pins, solder wire joint on the left and solder paste joint on the right
Featured image: the same six pins soldered two ways in this trial — wire on the left, paste on the right.

Wire and paste are not interchangeable processes that happen to use different consumables. On the same six pins, with the same laser and the same 1 mm spot, they produced different cycle times, different joint shapes and different amounts of residue. This note compares them with the numbers from a single test run rather than with generic advice.

The part, and the constraint that matters most

The workpiece is a radar sensor module. Two groups of three pins pass through oval ring pads, six joints in total. The board edge sits directly against a dark red plastic cavity — the housing recess that the radar assembly fits into.

Radar module before soldering, six through-hole pins in oval ring pads next to a plastic cavity
Before soldering: 2 × 3 pins in oval ring pads, with the plastic cavity running along the board edge. The sample was held with a temporary fixture.

That cavity is the real constraint. It sits within a few millimetres of the joint line, it is plastic, and it absorbs heat differently from copper. Any process chosen for this part has to keep its energy in the pad, not in the housing. The sample itself was fixed with a temporary measure during the trial, which is worth noting because repeatability of pin position is what makes a 1 mm spot land correctly.

Shared optics, identical for both runs

Laser power 200 W
Wavelength 915 nm
Fiber core 200 µm
Focal length / working distance 100 mm / 100 mm
Spot 1 mm, circular
Workpiece / head angle 0° / 90°
Ambient 20 °C, 45 % RH

Everything downstream of this table is a process decision, not an equipment change. That is the useful part of the comparison: the differences below come from how the solder was delivered, not from how the light was delivered.

Route A — solder wire: 1480 ms per joint

Wire was fed into the joint under the beam, with retraction at the end of each feed. The recorded parameters:

Alloy / flux SAC305, 3 % flux
Wire length per joint 5 mm
Peak temperature 360 °C
Heating time per joint 1480 ms

The program is worth reading closely, because it explains the cycle time. It is not a single heating pulse. The sequence feeds wire forward, heats in steps to 360 °C, feeds again for the fill, pulls the wire back, and only then ends the cycle. The retract move is the detail that matters in production: pulling the wire back at the end of the feed separates the molten tip from the wire, which controls how much solder stays on the pad and prevents a drawn-out spike as the head moves away.

Laser soldering program screen for the solder wire run, showing stepped temperature and feed, stop and retract actions
The wire program: stepped heating to 360 °C with forward feed, stop and retract actions in the same cycle.
Six laser soldered pins using solder wire, domed joints with solidification wrinkles
After the wire run: all six joints formed, with a domed profile and visible solidification wrinkles. Slight yellowing of flux at the joint edge; no obvious spatter.

Route B — solder paste: 2300 ms per joint

Paste was pre-deposited on the pads and then heated. Same alloy family, different flux load:

Alloy / flux SAC305 paste, 13 % flux
Deposition Pre-deposited on pad
Peak temperature 350 °C
Heating time per joint 2300 ms

The paste program has two temperature steps: 150 → 250 °C held for 1000 ms, then 250 → 350 °C held for 1300 ms. It reaches a lower peak than the wire run but takes 820 ms longer per joint, because the paste has to be brought through its whole reflow before the joint is complete, and the dwell times are set longer than the wire program’s heating steps.

Laser soldering program screen for the solder paste run with two stepped temperature ramps
The paste program: two stepped ramps, 150 → 250 °C for 1000 ms and 250 → 350 °C for 1300 ms.
Six laser soldered pins using solder paste, flatter joints with white flux residue rings
After the paste run: joints are flatter and spread wider, with a visible white residue band around each pad. One joint shows a shallow crater at its centre.

What the two runs actually differ in

Solder wire Solder paste
Cycle time per joint 1480 ms 2300 ms (×1.55)
Peak temperature 360 °C 350 °C
Flux content 3 % 13 %
Joint profile Domed, more solder Flatter, wider spread
Residue Light yellowing at the edge Clear white band around pads
Solderability OK OK

The report records both processes as solderable and lists both parameter sets. It does not give a yield figure, a pull strength or a void count, so this article does not either. The differences above are the ones visible in the parameters and in the photos.

Read the cycle time as a cost, not as a defect. 820 ms extra per joint on a six-joint module is 4.9 seconds per board. If the line runs one module every few seconds, that difference decides the station count. If the line is dominated by another process, it does not.

How to choose between them on a radar module

Choose wire when cycle time dominates and the joint can take a dome. The 3 % flux load leaves far less residue, which matters when the cavity next to the pins cannot be washed. The retract action gives repeatable solder volume without a dispensing step. The trade-off is that the feed motion takes time and the joint sits proud of the pad.

Choose paste when the pad geometry needs a flat, low-profile joint and deposition can be automated. Paste spread wider on these oval ring pads and produced a flatter fillet. But 13 % flux leaves a visible residue band, and on a part with a plastic cavity a few millimetres away, cleaning has to be planned into the line rather than added later.

Whichever route is chosen, the wire feed itself is a parameter in its own right — the relationship between feed rate, retract and joint quality is covered in how wire feeding rate affects the laser soldering joint.

What we would change before this goes to production

  1. Replace the temporary fixture. Six pins within a 1 mm spot’s reach of a plastic cavity leave no margin for position error. The fixture is the first thing to fix, not the power.
  2. Check the plastic cavity temperature. The report does not record it, and on a part this tight it should be measured on both routes, not assumed.
  3. Decide on cleaning with the process selection. Paste’s residue band is predictable, and it is easier to design the station in than to retrofit it.
  4. Bring the cycle time down before scaling. Both runs are described in the report as having room to improve on parameters, joint condition and cycle time; the 1480 ms wire cycle is the better starting point for that work.

FAQ

Is laser solder wire faster than laser solder paste?

In this trial, yes: 1480 ms per joint with wire against 2300 ms with paste, on the same pins with the same 200 W laser and 1 mm spot. The wire program is a shorter heating sequence, while the paste program has to carry the full reflow with two dwells.

Why does paste need a lower peak temperature but take longer?

The paste run peaked at 350 °C against 360 °C for wire, but each joint spent longer under the beam — 2300 ms versus 1480 ms. Reaching a lower peak still requires bringing the whole deposit through reflow, and the dwell times in the paste program were set longer.

Why does flux content matter so much here?

The wire run used 3 % flux and left only light yellowing at the joint edge. The paste used 13 % flux and left a clear white residue band around each pad. On a module with a plastic cavity close to the pins, that residue determines whether a cleaning station is required.

What does the wire retract action do?

It pulls the wire back at the end of the feed so the molten tip separates cleanly from the wire. That fixes how much solder remains on the pad and prevents a spike being drawn out as the head moves to the next pin.

Can both processes run on the same machine?

In this trial both ran on the same platform with identical optics — 200 W, 915 nm, 200 µm fiber, 100 mm focal length and working distance, 1 mm circular spot. Only the solder delivery and the program changed.

One-line takeaway: with the light held constant, wire bought 820 ms per joint and a much cleaner board; paste bought a flatter joint and a residue problem. Pick which one your line can live with.

Six pins next to a plastic cavity?

Send the pad drawing and the housing section. We will run wire and paste on the same laser soldering platform and return both parameter sets with photos, the way this note was built. Consumables: solder wire and lead-free solder paste.

Source: internal test report 20260326B, 26 March 2026 — radar sensor module, 2 × 3 through-hole pins in oval ring pads, 200 W / 915 nm, 200 µm fiber, 100 mm focal length and working distance, 1 mm circular spot, 20 °C / 45 % RH. Wire: SAC305, 3 % flux, 5 mm wire length, 360 °C peak, 1480 ms. Paste: SAC305, 13 % flux, 350 °C peak, 2300 ms. All parameters, photographs and conclusions are taken from that one test record; no yield, strength or void data is reported there and none is claimed here.

Need Help?

Tell us about your application — our engineers will recommend the right solution.

Talk to an Engineer